Inconel 718 is a precipitation hardened Ni-based superalloy for aerospace applications
where corrosion, creep and fatigue resistance are required. Additive manufacturing
(AM) enables production of new designs of weight-optimised components with
features not possible with traditional manufacturing techniques. However, components
produced by additive manufacturing contain some defects such as gas porosity
and lack of fusion defects (LOFD) which deteriorate the mechanical performance of
the components. Hot Isostatic Pressing (HIP) utilises a high pressure up to 200
MPa in combination with a high temperature of up to 2000°C in a gas atmosphere
to heal the defects in additively manufactured parts.
In this project, focus was placed on defect elimination in case of Inconel 718 components,
produced by powder bed fusion technologies. To do so, two sets of cylinders
(5 and 10 mm in diameter) were produced by laser powder bed fusion (LPBF) and
electron beam melting (EBM). The cylinders contain a designed 1-mm sphere filled
by un-molten powder in the centre of the sample. Pores contain processing gas,
that is Ar in case of LPBF and gas residues from the vacuum in case of EBM. The
specimens experienced 5 variants of HIPing cycles followed by 2 variants of heat
treatments. All HIPing cycles were done at 150 MPa pressure and temperature of
1120 and 1180°C for duration between 5 and 360 minutes in 5 different combinations.
Standard heat treatment for IN718 was performed inside HIP (pressurised
heat treatment) or at atmospheric pressure. The LPBF and EBM specimens responded
differently to the HIPing cycles. The HIPing cycles were not able to fully
heal all gas porosities in LPBF specimens at applied conditions. Specimens from
EBM were fully dense after HIPing for 1 hour. The LPBF specimens experience a
re-growth of Ar porosity during atmospheric heat treatment compared to pressurised
heat treatment in HIP. The microstructure inside the designed sphere is analysed in
terms of oxide films, nitride inclusions, and prior powder boundaries.
The designed sphere filled by powders was seen as a relatively large lack of fusion
defect, and this gave the possibility of following this defect during HIP and HT. The
grain structure and precipitation of different phases are compared to the solidification
microstructure achieved by laser and electron beam processes.
Beskrivning
Ämne/nyckelord
AM, LPBF, EBM, HIP, IN718, Argon porosity, porosity reopen, regrowth